淬火作用 的英文怎麼說
中文拼音 [cuìhuǒzuòyòng]
淬火作用
英文
quenching effect-
Features : hardened and precision - ground bedways, the spindle is supported with precision taper roller bearings, gears in the headstock are made of high - quality steel, hardened and ground, speed - changing levers driven by fan - shaped gears, operating easily, safe interlock and a overload safety devices in apron, electromagnetic braking, cooling and lighting devices are supplied
特點:床身導軌表面經淬火和精密磨削,主軸支撐採用精密圓錐滾子軸承,主軸箱內齒輪採用優質鋼並經表面淬火和磨削,變速機構採用扇型齒輪傳動,操作靈活方便,溜板箱設有安全互鎖裝置和過載保險機構,配有電磁剎車、冷卻及照明裝置。Product description : this series product has entire auto - lubrication systems and the ordinary two big kinds supplies to select, this machine major parts cancels the needle, cam and the ball bearing all uses the high quality import components, also selects the high quality steel products quenching heat treatment to the main stress components, the essential components uses special phosphorus processing, the foreign dew components all adopts special - purpose seal - up device and drains the oil the measure, therefore, entire causes machine throughout to locate the lubrication is reliable, the revolution is steady, under the high speed low chirp condition works
本系列產品具有全自動潤滑型及普通型兩大類以供選用,本機主要零件勾針,凸輪及滾珠均採用優質進口零件,對主要受力零件亦選用優質鋼材淬火熱處理,關鍵零件則採用專門磷化處理,對外露零件均採取專用密封裝置及排油措施,因此,使整機始終處于潤滑可靠,運轉平穩,高速低噪的條件下工作。Class1 : chemicals used in industry 、 science and photography 、 as well as in agriculture 、 horticulture and forestry 、 unprocessed artificial resins 、 unprocessed plastics 、 manures 、 fire extinguishing compositions 、 tempering and soldering preparations 、 chemical substances for preserving foodstuffs 、 tanning substances 、 adhesives used in industry
類別1 :用於工作、科學、攝影、農業、園藝、森林的化學品,未加工人造合成樹脂,未加工塑料物,肥料,滅火用合成物,淬火和金屬焊接用制劑,保存食用化學品,鞣料,工業用黏合劑。Class 1 chemicals used in industry, science and photography, as well as in agriculture, horticulture and forestry ; unprocessed artificial resins, unprocessed plastics ; manures ; fire extinguishing compositions ; tempering and soldering preparations ; chemical substances for preserving foodstuffs ; tanning substances ; adhesives used in industry
商標注冊類別1用於工作、科學、攝影、農業、園藝、森林的化學品,未加工人造合成樹脂,未加工塑料物,肥料,滅火用合成物,淬火和金屬焊接用制劑,保存食用化學品,鞣料,工業用黏合劑。Chemicals used in industry, science and photography, as well as in agriculture, horticulture and forestry ; unprocessed artificial resins, unprocessed plastics ; manures ; fire extinguishing compositions ; tempering and soldering preparations ; chemical substances for preserving foodstuffs ; tanning substances ; adhesives used in industry
用於工作科學攝影農業園藝森林的化學品,未加工人造合成樹脂,未加工塑料物,肥料,滅火用合成物,淬火和金屬焊接用制劑,保存食用化學品,鞣料,工業用黏合劑。Results of the experiments showed that the wear mechanisms of the sintered steel included abrasive wear, adhesive wear and fatigue wear, and it was the abrasive wear most important. it was the sintered steel mixed by ni, mo that was the best on the wear resistance, because of the great lot of bainite ; the sintered steel quenched and low temperature tempered mixed by mo, w that was the best on the wear resistance, because of the rigidity of the steel was the highest
實驗結果表明:本文中幾種燒結鋼的磨損機制均是由磨粒磨損、粘著磨損、和疲勞磨損共同作用的,且以磨粒磨損為主;在燒結態下,復合添加合金元素鎳、鉬的燒結鋼的耐磨性能最好,這是因為生成了大量的硬質相貝氏體;而淬火、低溫回火態下,則復合添加鉬、鎢的燒結鋼的耐磨性能最好,這是因為熱處理態下添加鉬、鎢的燒結鋼的硬度最高。The network carbide and acicular martensites that existed in the microstructure of the root grooves of the spline due to improper carburating and quenching process of the shafts, led to the initiation and propagation of the intergranular microcracks and were the main reason that caused the early fracture of the shafts
由於滲碳淬火工藝不當,在二軸花鍵槽根部的組織中產生了網狀破化物和粗大的針狀馬氏體,在外力作用下形成沿晶顯微裂紋並擴展,是導致二軸疲勞斷裂的主要原因。In chapter four, in our experiments, we selected four representative mould steels as samples. after laser heat treatment, the hardness of samples was measured by special instrument, microstructure was also photographed to be analyzed carefully. through these experiments, we also debated on the theories which explain the new phenomenon occurring in laser overlapping treatment
第二章:介紹了工業中的各種激光加工技術和激光加工系統,詳細說明了本實驗所使用的高功率激光加工系統;第三章:詳細敘述了激光淬火的機理和熱傳導數學模型;第四章:通過實驗,分析激光淬火后的模具鋼的硬化帶的硬度分佈及金相組織特性,同時對激光交疊熱處理的特點及形成機理都作了深入的探討。We studied the effect of laser quenching ( harden by phase transformation ) on some representative mould steels. through measuring the rigidity on the surface of samples treated by laser heat treatment, and through photographing microstructures of the steel surface, we find many reasons attribute to high hardness. these reasons include ultra - fine grains, high density dislocation and more content of carbon in martensite
我們研究的是激光淬火對幾種典型模具鋼的作用,通過對熱處理后的試樣的硬度分佈的測定,用金相和電鏡觀察金相組織的變化,認為激光熱處理產生高硬度的原因是晶粒細化、高的位錯密度和高的馬氏體含量。First, the research background of this dissertation is set forth, and summarized with the overview of the history and the current development of residual stress research, based on reading a lot of literatures, and summarized with the general situations of aircraft aluminum alloys quenching and numerical simulation, those are pointed out objective, significance, methods of this research
本文主要採用數值模擬、理論分析、實驗驗證等方法,對航空構件淬火殘余應力的產生及影響進行了研究。主要工作集中在以下幾個方面: 1 、闡述了本學位論文的選題背景,在查閱國內外研究文獻的基礎上,歸納總結了航空鋁合金淬火殘余應力的研究概況,給出了論文的主要研究目標、內容及方法。In this thesis, we studied the effect of laser heat treatment and overlapping treatment on mould steel, debated on the principle of laser heat treatment, and explained the new phenomenon observed in this experiment. to some degree, maybe our research is beneficial to the development of laser heat treatment technology in practice
本文的研究了激光淬火以及激光交疊熱處理對模具鋼性能的影響,分析了激光熱處理的機理,對實際工作會有一定的實際意義,激光淬火也會隨著激光器的發展有更廣闊的應用前景。Quenching and tempering were chosen to strengthen the material. the quenching temperature and time were adjusted based on the hardness measurement
選擇淬火和回火作為本課題的熱處理工藝,並用硬度法確定可行的淬火溫度和保溫時間。分享友人